Amorphous Polymer |
nD1 |
Poly(1,4-butadiene) |
1.539 |
Poly(1-butene) |
1.497 |
Poly(2,2,2-trifluoroethyl acrylate) |
1.409 |
Poly(2,2,2-trifluoroethyl methacrylate) |
1.418 |
Poly(2,2,3,3-tetrafluoropropyl
methacrylate) |
1.420 |
Poly(2,5-dimethyl-1,4-phenylene
ethylene) |
1.595 |
Poly(2,6,3',5'-tetrachloro bisphenol A
carbonate) |
1.598 |
Poly(2,6-dichlorostyrene) |
1.625 |
Poly(2,6-dimethyl-p-phenylene oxide),
PPO |
1.579 |
Poly(2-bromoethyl methacrylate) |
1.535 |
Poly(2-chloroethyl methacrylate) |
1.503 |
Poly(2-chlorostyrene) |
1.597 |
Poly(2-ethoxyethyl acrylate) |
1.474 |
Poly(2-ethoxyethyl methacrylate) |
1.495 |
Poly(2-hydroxyethyl methacrylate) |
1.507 |
Poly(2-methoxystyrene) |
1.585 |
Poly(2-methylstyrene) |
1.587 |
Poly(2-phenylethyl methacrylate) |
1.547 |
Poly(3-ethoxypropyl acrylate) |
1.462 |
Poly(3-methoxypropyl acrylate) |
1.483 |
Poly(4-bromophenyl methacrylate) |
1.596 |
Poly(4-methyl-1-pentene) |
1.462 |
Poly(4-methylstyrene) |
1.578 |
Poly(acrylic acid), PAA |
1.508 |
Poly(acrylonitrile) |
1.513 |
Poly(benzyl methacrylate) |
1.589 |
Poly(Bisphenol A carbonate), PC |
1.586 |
Poly(Bisphenol B carbonate) |
1.583 |
Poly(butyl acrylate), PBA |
1.465 |
Poly(butyl methacrylate) |
1.483 |
Poly(caprolactam), ylon 6 |
1.530 |
Polychloroprene (Neoprene) |
1.561 |
Poly(cyclohexyl methacrylate) |
1.507 |
Poly(dodecyl methacrylate) |
1.465 |
Poly(ethyl acrylate), PEA |
1.467 |
Poly(ethyl methacrylate) |
1.498 |
Poly(ethyl vinyl ether) |
1.463 |
Poly(ethylene glycol) |
1.458 |
Poly(ethylene terephthalate), PET |
1.575 |
Poly(ethylene) |
1.476 |
Poly(hexamethylene adipamide), Nylon 6,6 |
1.530 |
Poly(hexamethylene sebacamide), Nylon
6,10 |
1.539 |
Poly(hexyl methacrylate) |
1.481 |
Poly(hexyl vinyl ether) |
1.459 |
Poly(isobutene) |
1.507 |
Poly(isobutyl methacrylate) |
1.480 |
Poly(isobutyl vinyl ether) |
1.451 |
Polyisoprene |
1.521 |
Poly(isopropyl methacrylate) |
1.463 |
Polylactic acid, PLA |
1.465 |
Poly(methacrylonitrile) |
1.590 |
Poly(methyl acrylate), PMA |
1.476 |
Poly(methyl isopropenyl ketone) |
1.520 |
Poly(methyl methacrylate) |
1.491 |
Poly(methyl vinyl ether) |
1.458 |
Poly(N-benzyl methacrylamide) |
1.597 |
Poly(N-methyl-methacrylamide) |
1.529 |
Poly(N-methyl-methacrylamide) |
1.529 |
Poly(octyl vinyl ether) |
1.461 |
Poly(oxymethylene) |
1.453 |
Poly(pentyl vinyl ether) |
1.459 |
Poly(phenyl methacrylate) |
1.561 |
Poly(propyl methacrylate) |
1.484 |
Poly(propylene sulfide) |
1.596 |
Poly(p-xylene) |
1.669 |
Polystyrene, PS |
1.593 |
Polysulfone, PSU |
1.642 |
Poly(tert-butyl methacrylate) |
1.464 |
Poly(tetrafluoroethylene), PTFE |
1.356 |
Poly(tetrahydrofurfuryl methacrylate) |
1.508 |
Poly(vinyl acetate) |
1.484 |
Poly(vinyl alcohol) |
1.526 |
Poly(vinyl benzoate) |
1.561 |
Poly(vinyl butyral) |
1.485 |
Poly(vinyl chloride), PVC |
1.531 |
Poly(vinyl formate) |
1.476 |
Poly(vinyl methyl ketone) |
1.459 |
Poly(vinylidene chloride), PVDC |
1.615 |
Poly(vinylidene fluoride), PVDF |
1.426 |
Poly(ω-dodecanamide), Nylon 12 |
1.525 |